Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the the-events-calendar domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home/storm/sites/dev-imca-int-com-1/public/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the broken-link-checker domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home/storm/sites/dev-imca-int-com-1/public/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the woocommerce-eu-vat-number domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home/storm/sites/dev-imca-int-com-1/public/wp-includes/functions.php on line 6114
Damaged high pressure content gauge hoses on bail-outs - DEV imca
Skip to content

Damaged high pressure content gauge hoses on bail-outs

What happened?

During diving activities on two occasions in the same 24-hour period, a diver noticed that there was no pressure left in his bail-out bottle.  The decision was taken by the Dive Supervisor to recover the diver from the water, as per standard protocol.  After recovery, the bail-out bottle and appliances were checked, and it was found that the high pressure content gauge hose on the bail-out was damaged.

Both hoses were replaced for new hoses.

Damaged hose showed cuts in outer skin
Damaged hose showed a damaged outer skin near the ferrule

What went wrong?

The short interval in which these two incidents happened triggered an investigation which revealed the following:

  • There were two different types of damage:
    • cuts; most likely caused by sharp mussels and stones (illustration above left)
    • damage caused by bending and overstressing (illustration above right);
  • Both hoses were leak tested and found to be leaking through holes near the ferrule connector;
  • Both hoses were fitted with bend restrictors;
  • The hoses were maintained and tested in accordance with Code of practice for the initial and periodic examination, testing and certification of diving plant and equipment
  • The hoses were subjected to a regular visual inspection before every dive;
  • Both hoses were in use for up to 4 years and were regularly used.

What were the causes?

Investigation suggested that one type of HP hose is prone to damage near the ferule connector, caused by bending and stressing, regardless of the use of a bend restrictor present at this location.  The damage was not sustained in one single occasion but is believed to have developed over time.

What actions were taken?

There are different types of HP hoses on the market with specific characteristics:

  • Hose type 1: fatigue like damage may occur near the ferrule over time. When this damage occurs, it can lead to loss of the bail-out within a dive.  In order to reduce the risk of this type of damage occurring, annual replacement may be required, depending on usage.
  • Hose type 2: does not show the same fatigue damage development as the construction is more flexible and rugged.
Hose type 1
Hose type 2
  Hose type 1 Hose type 2
Appearance Thin, smooth, black, shiny Thick, black, dull-coloured
Dimensions Outside diameter 10.8mm Outside diameter 12.5mm
Composition 3 layers:

Thin layer, plastic-like type (shrink fit)

Soft woven middle layer

Rigid inner layer, hard plastic-like tube

3 layers:

Thick outer layer, rubber compound

Soft woven middle layer

Flexible thick inner layer, rubber compound

Other findings Layers can move freely from each other

Outer layer easily cut with knife

Stiff, hard to bend, inner layer tends to buckle

Layers are vulcanized to each other

In general, hard to cut with a knife

Easier to bend, smaller bending radius, inner layer does not tend to buckle

Members may wish to refer to:


IMCA Safety Flashes summarise key safety matters and incidents, allowing lessons to be more easily learnt for the benefit of all. The effectiveness of the IMCA Safety Flash system depends on Members sharing information and so avoiding repeat incidents. Please consider adding safetyreports@imca-int.com to your internal distribution list for safety alerts or manually submitting information on incidents you consider may be relevant. All information is anonymised or sanitised, as appropriate.

IMCA’s store terms and conditions (https://www.imca-int.com/legal-notices/terms/) apply to all downloads from IMCA’s website, including this document.

IMCA makes every effort to ensure the accuracy and reliability of the data contained in the documents it publishes, but IMCA shall not be liable for any guidance and/or recommendation and/or statement herein contained. The information contained in this document does not fulfil or replace any individual’s or Member's legal, regulatory or other duties or obligations in respect of their operations. Individuals and Members remain solely responsible for the safe, lawful and proper conduct of their operations.